Designation
Name |
The value |
Designation GOST Cyrillic |
03Х16Н15М3 |
Designation GOST Latin |
03X16H15M3 |
Transliteration |
03H16N15M3 |
By chemical elements |
03Cr16Н15Mo3 |
Name |
The value |
Designation GOST Cyrillic |
ЭИ844 |
Designation GOST Latin |
EI844 |
Transliteration |
EhI844 |
By chemical elements |
- |
Description
03KH16N15M3 steel is used: for the manufacture of welded structures operating under conditions of boiling phosphoric, sulfuric, 10% acetic acid and sulfuric acid media intended for long-term service at operating temperatures to +600 °C.
Note
Steel corrosion resistant austenitic class.
03KH16N15M3 steel has higher resistance to pitting than steel 0ЗХ17Н14М3.
Standards
Name |
Code |
Standards |
Classification, nomenclature and General rules |
В30 |
GOST 5632-72 |
Blanks. Of the workpiece. Slabs |
В31 |
OST 3-1686-90 |
Bars and shapes |
В32 |
TU 14-11-245-88 |
Steel pipes and fittings to them |
В62 |
TU 14-159-165-87, TU 14-3-219-89 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Cr |
Si |
Ni |
Fe |
Cu |
V |
Ti |
Mo |
W |
GOST 5632-72 |
≤0.03 |
≤0.015 |
≤0.02 |
≤0.8 |
15-17 |
≤0.6 |
14-16 |
Rest |
≤0.3 |
≤0.2 |
≤0.2 |
2.5-3 |
≤0.2 |
Fe is the basis.
From steel 03H16N15M3B differs absence in structure Nb.
Technological properties
Name |
The value |
Weldability |
Without restrictions. |