Steel 25Х18Н10В2 (ЭП610)

Designation

Name The value
Designation GOST Cyrillic 25Х18Н10В2
Designation GOST Latin 25X18H10B2
Transliteration 25H18N10V2
By chemical elements 25Cr18Н10W2
Name The value
Designation GOST Cyrillic ЭП610
Designation GOST Latin EP610
Transliteration EhP610
By chemical elements -

Description

25Х18Н10В2 steel is used: for the manufacture of nitride precision parts operating at temperatures up to +650 °C (continuous) and +700 °C (short-term).

Note

Steel 25Х18Н10В2 more technologically advanced than steel 4Х14Н14В2М: 25−40 hours of nitriding a layer with a depth of 0.12…0.25 mm.

Standards

Name Code Standards
Bars and shapes В32 TU 14-1-204-72

Chemical composition

Standard C S P Mn Cr Si Ni Fe W
TU 14-1-204-72 0.21-0.28 ≤0.03 ≤0.03 ≤0.7 17-19 0.3-0.8 9-11 Rest 2-2.5
Fe is the basis.
According to TU 14-1-204-72, the chemical composition is given for steel grade 25Х18Н10В2 (EP610). Deviations from the chemical composition are permissible: silicon ± 0.050%, chromium -0.50%, nickel + 0.50%, tungsten ± 0.10%, carbon + 0.010%. The presence of titanium up to 0.050%, aluminum up to 0.10%, copper to 0.25%, vanadium to 0.10%, molybdenum to 0.30%, niobium to 0.10%, cobalt to 0.50% sign.

Mechanical properties

Section, mm sT|s0,2, MPa σU, MPa d5, % y, % KCU, kJ/m2 HB, MPa
Bars on the other 14-1-204-72. The longitudinal samples. The untreated or after annealing 800-840 °C (exposure 2 hours), air cooling
≥313 ≥735 ≥20 ≥35 ≥690 ≤302

Description mechanical marks

Name Description
sT|s0,2 Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2%
σU Limit short-term strength
d5 Elongation after rupture
y The relative narrowing
KCU Toughness
HB Brinell hardness number