Designation
Name |
The value |
Designation GOST Cyrillic |
25ХГЛ |
Designation GOST Latin |
25XGL |
Transliteration |
25HGL |
By chemical elements |
25CrMn |
Description
25KHGL steel is used: for the manufacture of castings to various industrial purpose.
Standards
Name |
Code |
Standards |
Steel castings |
В82 |
GOST 977-88 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Cr |
Si |
Fe |
GOST 977-88 |
0.2-0.3 |
≤0.04 |
≤0.04 |
0.85-1.15 |
0.9-1.3 |
0.2-0.5 |
Rest |
Fe is the basis.
Mechanical properties
Section, mm |
sT|s0,2, MPa |
σU, MPa |
d |
y, % |
KCU, kJ/m2 |
Hardening in air, 890-910 °C + vacation at 620-660 °C, air cooling |
100 |
≥304 |
≥579 |
≥12 |
≥20 |
≥206 |
Description mechanical marks
Name |
Description |
sT|s0,2 |
Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2% |
σU |
Limit short-term strength |
d |
Elongation after rupture |
y |
The relative narrowing |
KCU |
Toughness |