Designation
Name |
The value |
Designation GOST Cyrillic |
35ХГЛ |
Designation GOST Latin |
35XGL |
Transliteration |
35HGL |
By chemical elements |
35CrMn |
Description
35KHGL steel is used: for the manufacture of castings to various industrial purpose.
Standards
Name |
Code |
Standards |
Steel castings |
В82 |
GOST 977-88 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Cr |
Si |
Fe |
GOST 977-88 |
0.3-0.45 |
≤0.04 |
≤0.04 |
0.6-0.9 |
0.5-0.8 |
0.5-0.75 |
Rest |
Fe is the basis.
Mechanical properties
Section, mm |
sT|s0,2, MPa |
σU, MPa |
d |
y, % |
KCU, kJ/m2 |
Hardening in air, 840-860 °C + vacation at 500-680 °C, air cooling |
100 |
≥383 |
≥726 |
≥10 |
≥20 |
≥167 |
Normalization at 850-880 °C + Vacation at 550-650 °C, air cooling |
100 |
≥334 |
≥628 |
≥14 |
≥25 |
≥137 |
Description mechanical marks
Name |
Description |
sT|s0,2 |
Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2% |
σU |
Limit short-term strength |
d |
Elongation after rupture |
y |
The relative narrowing |
KCU |
Toughness |