Steel 27KH5GSML

Designation

Name The value
Designation GOST Cyrillic 27Х5ГСМЛ
Designation GOST Latin 27X5GCML
Transliteration 27H5GSML
By chemical elements 27Cr5MnСMo

Description

27KH5GSML steel is used: for the manufacture of castings of high-loaded details of responsible use thickness and above of wall up to 50mm, working in conditions of impact loads and shock-abrasive wear.

Standards

Name Code Standards
Steel castings В82 GOST 977-88

Chemical composition

Standard C S P Mn Cr Si Fe Mo
GOST 977-88 0.24-0.28 ≤0.02 ≤0.02 0.9-1.2 5-5.5 0.9-1.2 Rest 0.55-0.6
Fe is the basis.

Mechanical properties

Section, mm sT|s0,2, MPa σU, MPa d5, % y, % KCU, kJ/m2
Normalization at 970-990 °C + vacation at 700-720 °C, air cooling + tempering air from 980-1000 °C + vacation at 200-220 °C, air cooling
100 ≥1177 ≥1472 ≥5 ≥20 ≥392

Description mechanical marks

Name Description
sT|s0,2 Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2%
σU Limit short-term strength
d5 Elongation after rupture
y The relative narrowing
KCU Toughness