Designation
Name |
The value |
Designation GOST Cyrillic |
30НКД |
Designation GOST Latin |
30HKD |
Transliteration |
30NKD |
By chemical elements |
30NiCoД |
Name |
The value |
Designation GOST Cyrillic |
30НКД-ВИ |
Designation GOST Latin |
30HKD-BI |
Transliteration |
30NKD-VI |
By chemical elements |
30NiCoД-ВIr |
Description
Alloy 30NKD used: for the manufacture of vacuum-tight junctions with refractory glass stamps C38−1 and for certain types of junctions with glass stamps C40−1.
Note
Alloy with a low CTE value.
Alloy with a CTE (to 3.3−4.6)·10-6 deg-1 in the temperature range from minus 60 to plus 400 °C.
Standards
Name |
Code |
Standards |
Classification, nomenclature and General rules |
В30 |
GOST 10994-74 |
Tape |
В34 |
GOST 14080-78 |
Wire, steel, alloy |
В73 |
GOST 14081-78 |
Bars and shapes |
В32 |
GOST 14082-78, TU 14-11-245-88 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Si |
Ni |
Fe |
Cu |
Co |
GOST 10994-74 |
≤0.05 |
≤0.015 |
≤0.015 |
≤0.4 |
≤0.3 |
29.5-30.5 |
Rest |
0.3-0.5 |
13-14.2 |
Fe is the basis.
Mechanical properties
Section, mm |
σU, MPa |
Cold-rolled steel strip according to GOST 14080-78 on delivery |
0.1-2.5 |
≤930 |
Description mechanical marks
Name |
Description |
σU |
Limit short-term strength |
Physical characteristics
Temperature |
r, kg/m3 |
a, 10-6 1/°C |
20 |
8200 |
- |
-100 |
- |
56 |
-80 |
- |
55 |
-60 |
- |
53 |
-40 |
- |
51 |
-20 |
- |
50 |
100 |
- |
46 |
200 |
- |
44 |
300 |
- |
40 |
400 |
- |
45 |
500 |
- |
65 |
600 |
- |
82 |
700 |
- |
95 |
800 |
- |
107 |
A description of the physical symbols
Name |
Description |
Е |
The normal elasticity modulus |
l |
Coefficient of thermal conductivity |
Technological properties
Name |
The value |
Frost |
Tape x/K alloy 30NKD (30NKD-VI) according to GOST 14080-78 and wire cold-drawn according to GOST 14081-78 should be hardy to minus 70 °C. |
The temperature of the inflection point |
≥390 °C |