Designation
Name |
The value |
Designation GOST Cyrillic |
БрБ2 |
Designation GOST Latin |
BpB2 |
Transliteration |
BrB2 |
By chemical elements |
BaBe2 |
Description
Bronze Brb2 used: for the manufacture of semi-finished products (strips, sheets, bars, tubes and wire); springs and elastic sensing elements in instruments, spring details of responsible destination; wear-resistant parts of all kinds; non-sparking tools.
Note
Brb2 beryllium bronze has high strength and wear resistance, good sliding properties, very good deformability in the hardened state, the average electrical conductivity and thermal conductivity.
Analog bronze Brb2 at CMEA 377−76 is bronze CuBe2Ni (Co).
Standards
Name |
Code |
Standards |
Wire from nonferrous metals and their alloys |
В74 |
GOST 15834-77, OST 4.021.108-92 |
Bars |
В55 |
GOST 15835-2013, OST 4.021.024-92 |
Sheets and strips |
В53 |
GOST 1789-2013, OST 4.021.069-92 |
Non-ferrous metals, including rare, and their alloys |
В51 |
GOST 18175-78, GOST 28873-90, OST 4.021.009-92, TU 48-21-5062-89 |
Tape |
В54 |
OST 4.021.082-92, TU 48-0812-12-89, TU 48-0812-15-90, TU 48-0812-26-89, TU 48-21-265-87, TU 48-21-743-92 |
Processing of metals by pressure. Forgings |
В03 |
ST ЦКБА 010-2004 |
Chemical composition
Standard |
Si |
Ni |
Fe |
Cu |
Al |
Pb |
Be |
GOST 18175-78 |
≤0.15 |
0.2-0.5 |
≤0.15 |
Rest |
≤0.15 |
≤0.005 |
1.8-2.1 |
Cu is the basis.
According to GOST 18175-78, the total mass fraction of normalized impurities is ≤ 0.50%.
Mechanical properties
Section, mm |
sT|s0,2, MPa |
σU, MPa |
d5, % |
d |
d10 |
HB, MPa |
HV, MPa |
Strip 1,0-6,0 mm in the delivery state on the EAST 4.021.069-92 (samples transverse) |
- |
- |
390-590 |
- |
- |
≥30 |
- |
≥130 |
- |
- |
640-930 |
- |
- |
≥2.5 |
- |
≥170 |
Strip or tape according to GOST 1789-2013, OST 4.021.082-92. Hardening in air, 305-315 °C (exposure for 2.5 hours + warm-up time of charge) + the Deformation of 30-40 % |
0.15-0.25 |
- |
590-880 |
- |
- |
- |
- |
≥170 |
0.15 |
- |
- |
- |
- |
- |
- |
≥170 |
0.25 |
- |
640-930 |
- |
- |
≥2.5 |
- |
≥170 |
Strip or tape according to GOST 1789-2013, OST 4.021.082-92. Hardening in air, 305-315 °C (extract 3 hours + warm-up time of the charge) |
0.15-0.25 |
- |
390-590 |
- |
- |
≥20 |
- |
≤130 |
0.15 |
- |
- |
- |
- |
- |
- |
≤130 |
0.25 |
- |
390-590 |
- |
- |
≥30 |
- |
≤130 |
Strip or tape according to GOST 1789-2013. Hardening in air, 305-315 °C (exposure for 2.5 hours + warm-up time of charge) + the Deformation of 30-40 % + Aging (dispersion hardening) |
0.15-0.25 |
- |
1130-1570 |
- |
- |
- |
- |
≥360 |
0.15 |
- |
- |
- |
- |
- |
- |
≥360 |
0.25 |
- |
1170-1570 |
- |
- |
≥1.5 |
- |
≥360 |
Strip or tape according to GOST 1789-2013. Hardening in air, 305-315 °C (extract 3 hours + warm-up time of charge) + Aging (dispersion hardening) |
0.15-0.25 |
- |
1080-1470 |
- |
- |
- |
- |
≥330 |
0.15 |
- |
- |
- |
- |
- |
- |
≥330 |
0.25 |
- |
1130-1470 |
- |
- |
≥2 |
- |
≥330 |
Wire soft (tempered), solid (cold-worked after quenching) in the delivery state according to GOST 15834-77. Heating for hardening is to 770-790 °C, exposure for 10-20 min., rapid cooling in water |
0.06-0.08 |
≥235 |
343-686 |
- |
15-60 |
- |
- |
≥100 |
0.1-1 |
≥235 |
392-637 |
- |
20-60 |
- |
- |
≥100 |
1.1-5 |
≥235 |
392-637 |
- |
25-60 |
- |
- |
≥100 |
5.5-12 |
≥235 |
392-588 |
- |
30-60 |
- |
- |
≥100 |
0.06-0.5 |
≥735 |
931-1372 |
- |
- |
- |
- |
≥180 |
0.55-1 |
≥735 |
833-1274 |
- |
- |
- |
- |
≥180 |
1.1-5 |
≥735 |
735-1176 |
- |
- |
- |
- |
≥180 |
5.5-12 |
≥735 |
735-1078 |
- |
- |
- |
- |
≥180 |
The wire is subjected to a dispersion hardening of the mild (tempered) and hard (cold-worked after quenching) States in the state of delivery according to GOST 15834-77. Heating for hardening is to 770-790 °C, exposure for 10-20 min., rapid cooling in water + Aging (dispersion hardening) at 310-330 °C, aging 3h. |
0.06-0.9 |
≥1078 |
1078-1470 |
- |
- |
- |
- |
≥320 |
1-12 |
≥1078 |
1078-1568 |
- |
- |
- |
- |
≥320 |
0.06-12 |
≥1372 |
≥1176 |
- |
≥1 |
- |
- |
≥360 |
Cold-drawn wire for the manufacture of parts and springs as supplied by OST 4.021.108-92 (longitudinal samples, indicated the relative elongation δ1) |
0.1-1 |
- |
392-637 |
- |
20-45 |
- |
- |
- |
1.2-5 |
- |
392-637 |
- |
25-60 |
- |
- |
- |
5.6-12 |
- |
392-588 |
- |
30-60 |
- |
- |
- |
0.1-0.5 |
- |
931-1372 |
- |
- |
- |
- |
- |
0.6-1 |
- |
833-1274 |
- |
- |
- |
- |
- |
1.2-5 |
- |
735-1176 |
- |
- |
- |
- |
- |
5.6-12 |
- |
735-1080 |
- |
- |
- |
- |
- |
Round bars pressed extra virgin in the state of delivery according to GOST 15835-2013 |
42-100 |
- |
≥440 |
≥20 |
- |
- |
- |
- |
Round bars, drawn, in the delivery state on the EAST 4.021.024-92, GOST 15835-2013 (longitudinal samples) |
5-40 |
- |
390-590 |
≥25 |
- |
- |
100-150 |
- |
16-40 |
- |
640-880 |
≥1 |
- |
- |
≥150 |
- |
5-15 |
- |
740-980 |
≥1 |
- |
- |
≥150 |
- |
Round bars, drawn, after dispersive hardening (aging) according to GOST 15835-70 (longitudinal samples, on delivery, rate is what condition aged samples) |
- |
- |
≥1080 |
≥2 |
- |
- |
- |
≥320 |
- |
- |
≥1180 |
≥2 |
- |
- |
- |
≥340 |
Description mechanical marks
Name |
Description |
sT|s0,2 |
Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2% |
σU |
Limit short-term strength |
d5 |
Elongation after rupture |
d |
Elongation after rupture |
d10 |
Elongation after rupture |
HB |
Brinell hardness number |
HV |
The Vickers hardness |
Physical characteristics
Temperature |
Е, HPa |
r, kg/m3 |
l, W/(m · °C) |
R, Mr. · m |
20 |
6-132 |
8200 |
84 |
70-200 |
A description of the physical symbols
Name |
Description |
Е |
The normal elasticity modulus |
r |
Density |
l |
Coefficient of thermal conductivity |
R |
UD. the resistivity |
С |
Specific heat |