Designation
Name |
The value |
Designation GOST Cyrillic |
БрБ1,7НТ |
Designation GOST Latin |
BpB1,7HT |
Transliteration |
BrB17NT |
By chemical elements |
BaBe1,7NiTe |
Name |
The value |
Designation GOST Cyrillic |
БрБНТ1,7 |
Designation GOST Latin |
BpBHT1,7 |
Transliteration |
BrBNT17 |
By chemical elements |
BaBeNiTe1,7 |
Description
Bronze БрБ1,7НТ used: for the manufacture of springs and elastic sensing elements in the instrument.
Note
Bronze БрБ1,7НТ (Brbnt1,7) has high strength and wear resistance, good sliding properties, very good deformability in the hardened state.
Standards
Name |
Code |
Standards |
Non-ferrous metals, including rare, and their alloys |
В51 |
GOST 18175-78 |
Tubes of non-ferrous metals and alloys |
В64 |
TU 48-21-426-83 |
Chemical composition
Standard |
Si |
Ni |
Fe |
Cu |
Al |
Ti |
Pb |
Be |
GOST 18175-78 |
≤0.15 |
0.2-0.4 |
≤0.15 |
Rest |
≤0.15 |
0.1-0.25 |
≤0.005 |
1.6-1.85 |
Cu is the basis.
According to GOST 18175-78, the total mass fraction of normalized impurities is ≤ 0.50%.
Mechanical properties
Section, mm |
σU, MPa |
d5, % |
HV, MPa |
Strip or tape according to GOST 1789-2013. Hardening in air, 305-315 °C (exposure for 2.5 hours + warm-up time of charge) + the Deformation of 30-40 % |
0.15-0.25 |
590-930 |
- |
≥150 |
0.15 |
- |
- |
≥150 |
0.25 |
590-930 |
≥2.5 |
≥150 |
Strip or tape according to GOST 1789-2013. Hardening in air, 305-315 °C (exposure for 2.5 hours + warm-up time of charge) + the Deformation of 30-40 % + Aging (dispersion hardening) |
0.15-0.25 |
1080-1470 |
- |
≥340 |
0.15 |
- |
- |
≥340 |
0.25 |
1080-1470 |
≥2 |
≥340 |
Description mechanical marks
Name |
Description |
σU |
Limit short-term strength |
d5 |
Elongation after rupture |
HV |
The Vickers hardness |
Physical characteristics
Temperature |
Е, HPa |
r, kg/m3 |
l, W/(m · °C) |
R, Mr. · m |
20 |
128 |
8200 |
966 |
90 |
A description of the physical symbols
Name |
Description |
Е |
The normal elasticity modulus |
l |
Coefficient of thermal conductivity |
R |
UD. the resistivity |