Designation
Name |
The value |
Designation GOST Cyrillic |
НП2 |
Designation GOST Latin |
HP2 |
Transliteration |
NP2 |
By chemical elements |
NiП2 |
Description
Nickel NP2 is used: for the production of semi-finished products (strips, sheets, strips, pipes, wire, drawn (5−40 mm) and hot rolled (42−90 mm) bars); elements of instrumentation and engineering; joints of sheet structures with a thickness of 2.0 to 6.0 mm, working with radioactive environment; as a cladding layer in the manufacture of hot-rolled dual-layer corrosion-resistant sheets; tape thickness of 0.05−2.0 mm, used in electronics and other industries.
Standards
Name |
Code |
Standards |
Sheets and strips |
В33 |
GOST 10885-85, TU 26-929-40-93 |
Bars |
В55 |
GOST 13083-77 |
Tape |
В54 |
GOST 2170-73, OST 4.021.084-92, TU 48-21-567-78 |
Wire from nonferrous metals and their alloys |
В74 |
GOST 2179-75, OST 4.021.109-92, TU 48-21-710-80 |
Non-ferrous metals, including rare, and their alloys |
В51 |
GOST 28873-90, GOST 492-2006, OST 4.021.009-92 |
Sheets and strips |
В53 |
GOST 6235-91 |
Welding and cutting metals. Soldering, riveting |
В05 |
OST 95 10441-2002 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Si |
Ni |
Fe |
Cu |
As |
Zn |
Sn |
Sb |
Pb |
Bi |
Mg |
Cd |
Ni+Co |
GOST 492-2006 |
≤0.1 |
≤0.005 |
≤0.002 |
≤0.05 |
≤0.15 |
Rest |
≤0.1 |
≤0.1 |
≤0.002 |
≤0.007 |
≤0.002 |
≤0.002 |
≤0.002 |
≤0.002 |
≤0.1 |
≤0.002 |
≥99.5 |
Ni is the basis.
According to GOST 492-2006, the total mass fraction of impurities is ≤ 0.50%. Due to the mass fraction of nickel, the mass fraction of cobalt in the amount of ≤ 0.20% is allowed. Upon agreement of the manufacturer with the consumer, the mass fraction of zinc in the amount of ≤ 0.020% is allowed.
Mechanical properties
Section, mm |
σU, MPa |
d5, % |
d |
d10 |
Hot-rolled sheets, hot rolled and cold rolled strip in the delivery state according to GOST 6235-91 (samples transverse) |
|
≥370 |
≥15 |
- |
- |
|
≥370 |
≥35 |
- |
- |
|
≥540 |
≥2 |
- |
- |
Cold-rolled steel strip as supplied by the 2170-73 GOST, OST 4.021.084-92 (samples transverse) |
- |
≥390 |
≥35 |
- |
≥32 |
- |
≥440 |
≥12 |
- |
≥10 |
- |
≥540 |
≥3 |
- |
≥2 |
Cold-drawn wire in soft (annealed) and hard (cold-worked) condition of delivery on the OST 4.021.109-92 (longitudinal samples) |
0.3-0.4 |
≥420 |
- |
≥18 |
- |
0.5-1 |
390-590 |
- |
≥20 |
- |
1.2-1.6 |
390-530 |
- |
≥26 |
- |
2-12 |
≥370 |
- |
≥26 |
- |
0.3-0.5 |
780-1080 |
- |
- |
- |
0.6-1 |
740-980 |
- |
- |
- |
1.2-5 |
690-880 |
- |
- |
- |
5.6-12 |
590-830 |
- |
- |
- |
The bar in the state of delivery (longitudinal samples) |
42-90 |
≥440 |
≥10 |
- |
≥8 |
5-40 |
≥370 |
≥30 |
- |
≥26 |
5-40 |
≥540 |
≥5 |
- |
≥3 |
Description mechanical marks
Name |
Description |
σU |
Limit short-term strength |
d5 |
Elongation after rupture |
d |
Elongation after rupture |
d10 |
Elongation after rupture |
Physical characteristics
Temperature |
r, kg/m3 |
20 |
8850 |
A description of the physical symbols
Name |
Description |
Е |
The normal elasticity modulus |
l |
Coefficient of thermal conductivity |
R |
UD. the resistivity |
С |
Specific heat |
Technological properties
Name |
The value |
Weldability |
Automatic arc welding with non-consumable electrode in a continuous mode, manual argon arc welding with non-consumable electrode (filler or without filler material). |