Steel 12KH19N7G2SAL

Designation

Name The value
Designation GOST Cyrillic 12Х19Н7Г2САЛ
Designation GOST Latin 12X19H7G2CAL
Transliteration 12H19N7G2SAL
By chemical elements 12Cr19Н7Mn2СN

Description

12KH19N7G2SAL steel is used: for the manufacture of castings to various industrial purpose.

Note

Steel corrosion resistant austenitic-ferritic class. Steel corrosion in air, nitric acid, very dilute sulfuric acid and dilute or weak organic acids.

Standards

Name Code Standards
Steel castings В82 GOST 977-88

Chemical composition

Standard C S P Mn Cr Si Ni Fe N
GOST 977-88 ≤0.12 ≤0.04 ≤0.04 ≤2 18-20 ≤1.5 6-8 Rest 0.1-0.2
Fe is the basis.

Mechanical properties

Section, mm sT|s0,2, MPa σU, MPa d y, % KCU, kJ/m2
Casting. Quenching in water or air from 1050-1100 °C
100 ≥240 ≥481 ≥20 ≥30 ≥590

Description mechanical marks

Name Description
sT|s0,2 Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2%
σU Limit short-term strength
d Elongation after rupture
y The relative narrowing
KCU Toughness