Steel 50Г23Х4ФВ7 (48ВННК-2)

Designation

Name The value
Designation GOST Cyrillic 50Г23Х4ФВ7
Designation GOST Latin 50G23X4FB7
Transliteration 50G23H4FV7
By chemical elements 50Mn23Cr4VW7
Name The value
Designation GOST Cyrillic 48ВННК-2
Designation GOST Latin 48BHHK-2
Transliteration 48VNNK-2
By chemical elements 48WННCo-2

Description

50Г23Х4ФВ7 steel is used: for the manufacture of forged and rolled round and square steel billets of open smelting and electroslag remelting (ESR); hull structures of ships, vessels and goods marine equipment (rotors, casings and other parts gyroscopic devices).

Note

Low high strength austenitic steel.
Magnetic permeability μ ≤ 1,002 GS/E.

Standards

Name Code Standards
Castings, non-ferrous metals and alloys В84 RD 9257-76
Bars and shapes В32 TU 14-1-214-72

Chemical composition

Standard C S P Mn Cr Si Fe V W
RD 9257-76 0.44-0.52 ≤0.025 ≤0.035 22-23 3-4.5 ≤0.6 Rest 1.25-1.55 6.7-7.5
Fe is the basis.
According to RD 9257-76 the chemical composition is given for steel 50Г23Х4ФВ7 and 50Г23Х4ФВ7-Ш.

Mechanical properties

sT|s0,2, MPa σU, MPa d5, % y, % KCU, kJ/m2
Steel 50Г23Х4ФВ7-sh. Without heat treatment. Bars hot rolled round 50-70 mm, round and square forged 100-150 mm
≥1080 ≥1226 ≥8 ≥12 ≥196
Steel 50Г23Х4ФВ7. Without heat treatment. Bars hot rolled round 30-70 mm, 100-150 mm forged round, forged square cross-section of 90-180 mm
≥1080 ≥1226 ≥5 ≥8 -

Description mechanical marks

Name Description
sT|s0,2 Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2%
σU Limit short-term strength
d5 Elongation after rupture
y The relative narrowing
KCU Toughness

Physical characteristics

Temperature Е, HPa r, kg/m3 l, W/(m · °C) a, 10-6 1/°C
20 181 8100 - -
200 - - 1717 -
300 - - 1926 -
400 - - 2177 -
100 - - - 1300

A description of the physical symbols

Name Description
r Density
l Coefficient of thermal conductivity
R UD. the resistivity