Alloy KHN60JU (ЭИ559А)

Designation

Name The value
Designation GOST Cyrillic ХН60Ю
Designation GOST Latin XH60Ju
Transliteration HN60Yu
By chemical elements CrNi60Al
Name The value
Designation GOST Cyrillic ЭИ559А
Designation GOST Latin EI559A
Transliteration EhI559A
By chemical elements -

Description

Alloy KHN60JU used: for the manufacture of sheet metal components for turbines operating at moderate voltages, parts, gas pipeline systems, equipment with limited service life at 1100 °C and short service life at 1250 °C.

Note

Alloy, heat-resistant and heat-resistant Nickel-based. The recommended maximum operating temperature for a limited time — 1200 °C. the Temperature of beginning of intensive scaling in air — more than 1250 °C.

Standards

Name Code Standards
Classification, nomenclature and General rules В30 GOST 5632-72
Blanks. Of the workpiece. Slabs В31 OST 3-1686-90
Bars and shapes В32 TU 14-11-245-88

Chemical composition

Standard C S P Mn Cr Si Ni Fe Cu Al Ti Mo Ce Ba
GOST 5632-72 ≤0.1 ≤0.02 ≤0.02 ≤0.3 15-18 ≤0.8 55-58 Rest ≤0.3 2.6-3.5 ≤0.2 ≤0.3 ≤0.03 ≤0.1
Ni is the basis.

Mechanical properties

Section, mm sT|s0,2, MPa σU, MPa y, %
Without heat treatment
≥4 360 720 50

Description mechanical marks

Name Description
sT|s0,2 Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2%
σU Limit short-term strength
y The relative narrowing

Physical characteristics

Temperature Е, HPa r, kg/m3 l, W/(m · °C) a, 10-6 1/°C
20 210 7900 - -
800 169 - 402 1518
100 - - 105 1228
200 - - 13 1308
300 - - 159 1342
400 - - 196 142
500 - - 24 1422
600 - - 293 1459
700 - - 345 1511
900 - - 474 1588

A description of the physical symbols

Name Description
Е The normal elasticity modulus
r Density
l Coefficient of thermal conductivity

Technological properties

Name The value
Weldability without restrictions