Designation
Name |
The value |
Designation GOST Cyrillic |
15Х18СЮ |
Designation GOST Latin |
15X18CJu |
Transliteration |
15H18SYu |
By chemical elements |
15Cr18СAl |
Name |
The value |
Designation GOST Cyrillic |
ЭИ484 |
Designation GOST Latin |
EI484 |
Transliteration |
EhI484 |
By chemical elements |
- |
Description
15KH18SJU steel is used: for the manufacture of parts and tubes of pyrolysis plants, equipment.
Note
Heat-resistant steel of the ferritic class.
Temperature intense scaling in air +1050 °C.
Stable in sulfur-containing environments.
Standards
Name |
Code |
Standards |
Classification, nomenclature and General rules |
В30 |
GOST 5632-72 |
Bars and shapes |
В32 |
GOST 5949-75, TU 14-11-245-88 |
Blanks. Of the workpiece. Slabs |
В31 |
OST 3-1686-90 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Cr |
Si |
Ni |
Fe |
Cu |
Al |
V |
Ti |
Mo |
W |
GOST 5632-72 |
≤0.15 |
≤0.025 |
≤0.035 |
≤0.8 |
17-20 |
1-1.5 |
≤0.6 |
Rest |
≤0.3 |
0.7-1.2 |
≤0.2 |
≤0.2 |
≤0.3 |
≤0.2 |
Fe is the basis.
Mechanical properties
Section, mm |
sT|s0,2, MPa |
σU, MPa |
d5, % |
y, % |
Bars hot rolled and forged according to GOST 5949-75. Annealing at 800-850 °C, cooling in air or in water |
|
≥295 |
≥490 |
≥20 |
≥50 |
Description mechanical marks
Name |
Description |
sT|s0,2 |
Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2% |
σU |
Limit short-term strength |
d5 |
Elongation after rupture |
y |
The relative narrowing |